Stainless-Steel-Fasteners-Mechanical-Properties
Mechanical properties - Stainless Steel Fasteners
Screws and Bolts up to M6 | |||||
Type | Grade | Nominal Size | Property Class | ||
50 | 70 | 80 | |||
Minimum Breaking Torque N/mm² | |||||
Austenitic | A1 A2 A4 | M1.6 | 0.15 | 0.2 | 0.27 |
M2 | 0.3 | 0.4 | 0.56 | ||
M2.5 | 0.6 | 0.9 | 1.2 | ||
M3 | 1.1 | 1.6 | 2.1 | ||
M4 | 2.7 | 3.8 | 4.9 | ||
M5 | 5.5 | 7.8 | 10 |
Screws, Bolts and Nuts from M6 | |||||||
Type | Grade | Property Class | Nominal Size | Bolts and Screws | Nuts | ||
Minimum Tensile Strength N/mm² | Minimum Proof Stress N/mm² | Minimum Elongation at fracture mm | Proof Load Stress (sp) N/mm² | ||||
Austenitic | A1 A2 A4 | 50 | M6 - M39 | 500 | 210 | 0.6 x Nom. Dia. | 500 |
70 | M6 - M20 | 700 | 450 | 0.4 x Nom. Dia. | 700 | ||
80 | M6 - M20 | 800 | 600 | 0.3 x Nom. Dia. | 800 |
Information is for guidance only and is correct to the best of our knowledge. The customer must satisfy themselves with the performance of the fastener and validity of the data.